{"id":8123,"date":"2026-05-01T04:25:49","date_gmt":"2026-05-01T08:25:49","guid":{"rendered":"https:\/\/plastisol-inks.com\/?p=8123"},"modified":"2026-05-07T04:54:34","modified_gmt":"2026-05-07T08:54:34","slug":"%e3%83%97%e3%83%a9%e3%82%b9%e3%83%81%e3%82%be%e3%83%ab%e3%82%a4%e3%83%b3%e3%82%af%e7%a1%ac%e5%8c%96%e3%82%ac%e3%82%a4%e3%83%892026-%e5%a4%a7%e9%87%8f%e5%8d%b0%e5%88%b7%e6%b8%a9%e5%ba%a6%e3%83%88","status":"publish","type":"post","link":"https:\/\/plastisol-inks.com\/ja\/plastisol-ink-curing-guide-2026-bulk-printing-temperature-troubleshooting\/","title":{"rendered":"\u30d7\u30e9\u30b9\u30c1\u30be\u30eb\u30a4\u30f3\u30af\u304c\u5b8c\u5168\u306b\u786c\u5316\u3057\u306a\u3044\u5834\u5408\u306f\uff1f\u5927\u91cf\u5370\u5237\u306e\u305f\u3081\u306e\u6e29\u5ea6\u30ac\u30a4\u30c9"},"content":{"rendered":"<div class=\"wp-block-rank-math-toc-block\" id=\"rank-math-toc\"><h2>\u76ee\u6b21<\/h2><nav><ul><li><a href=\"#why-we-wrote-this-the-solution-expert-perspective\">\u3053\u306e\u8a18\u4e8b\u3092\u66f8\u3044\u305f\u7406\u7531\uff1a\u30bd\u30ea\u30e5\u30fc\u30b7\u30e7\u30f3\u5c02\u9580\u5bb6\u306e\u8996\u70b9<\/a><\/li><li><a href=\"#the-2026-bulk-printing-cure-table\">2026\u5e74\u30d0\u30eb\u30af\u5370\u5237\u786c\u5316\u8868<\/a><\/li><li><a href=\"#how-to-get-started-calibrating-for-bulk\">\u59cb\u3081\u65b9\uff1a\u30d0\u30eb\u30af\u306e\u30ad\u30e3\u30ea\u30d6\u30ec\u30fc\u30b7\u30e7\u30f3<\/a><ul><li><a href=\"#1-the-stretch-test-the-quick-check\">1. \u30b9\u30c8\u30ec\u30c3\u30c1\u30c6\u30b9\u30c8\uff08\u30af\u30a4\u30c3\u30af\u30c1\u30a7\u30c3\u30af\uff09<\/a><\/li><li><a href=\"#2-the-wash-test-the-gold-standard\">2\uff0e\u6d17\u6d44\u30c6\u30b9\u30c8\uff08\u30b4\u30fc\u30eb\u30c9\u30b9\u30bf\u30f3\u30c0\u30fc\u30c9\uff09<\/a><\/li><li><a href=\"#3-verification-of-2026-standards\">3\uff0e2026\u5e74\u898f\u683c\u306e\u691c\u8a3c<\/a><\/li><\/ul><\/li><li><a href=\"#best-practice-managing-the-heat-sink-effect\">Best Practice: Managing the &#8220;Heat Sink&#8221; Effect<\/a><\/li><li><a href=\"#solving-the-cracking-mystery\">Solving the &#8220;Cracking&#8221; Mystery<\/a><\/li><li><a href=\"#fa-qs-from-our-global-partners\">\u30b0\u30ed\u30fc\u30d0\u30eb\u30d1\u30fc\u30c8\u30ca\u30fc\u304b\u3089\u306e\u3088\u304f\u3042\u308b\u8cea\u554f<\/a><ul><li><a href=\"#faq-question-1776925767849\">Q1. \u5927\u91cf\u6ce8\u6587\u306e\u5834\u5408\u3001\u7c21\u5358\u306a\u30d2\u30fc\u30c8\u30ac\u30f3\u3067\u30d7\u30e9\u30b9\u30c1\u30be\u30eb\u3092\u786c\u5316\u3055\u305b\u308b\u3053\u3068\u306f\u3067\u304d\u307e\u3059\u304b\uff1f<\/a><\/li><li><a href=\"#faq-question-1776925804543\">Q2. \u306a\u305c\u767d\u30a4\u30f3\u30af\u306f\u5265\u304c\u308c\u308b\u306e\u306b\u3001\u9ed2\u30a4\u30f3\u30af\u306f\u5265\u304c\u308c\u306a\u3044\u306e\u3067\u3059\u304b\uff1f<\/a><\/li><li><a href=\"#faq-question-1776925825005\">Q3. \u786c\u5316\u30d7\u30ed\u30bb\u30b9\u4e2d\u306b\u30a8\u30cd\u30eb\u30ae\u30fc\u3092\u7bc0\u7d04\u3059\u308b\u65b9\u6cd5\u306f\u3042\u308a\u307e\u3059\u304b\uff1f<\/a><\/li><li><a href=\"#faq-question-1776925869161\">Q4. \u30a4\u30f3\u30af\u3092\u904e\u5ea6\u306b\u786c\u5316\u3055\u305b\u308b\u3068\u3069\u3046\u306a\u308a\u307e\u3059\u304b\uff1f<\/a><\/li><li><a href=\"#faq-question-1776925932430\">Q5. \u6e7f\u5ea6\u306f\u4e7e\u71e5\u6a5f\u306e\u8a2d\u5b9a\u306b\u3069\u306e\u3088\u3046\u306b\u5f71\u97ff\u3057\u307e\u3059\u304b\uff1f<\/a><\/li><\/ul><\/li><li><a href=\"#final-thoughts-from-hong-rui-sheng\">\u30db\u30f3\u30fb\u30eb\u30a4\u30b7\u30a7\u30f3\u304b\u3089\u306e\u6700\u5f8c\u306e\u8a00\u8449<\/a><\/li><\/ul><\/nav><\/div>\n\n\n\n<p>If you&#8217;ve ever pulled a batch of shirts off the belt only to have a customer call two weeks later complaining that the design is flaking off like old paint, you\u2019ve hit the &#8220;undercure&#8221; wall. At <strong><a href=\"https:\/\/plastisol-inks.com\/ja\/\">\u30db\u30f3\u30fb\u30eb\u30a4\u30b7\u30a7\u30f3<\/a><\/strong>, we&#8217;ve seen it happen to the best shops.<\/p>\n\n\n\n<p><strong>The short answer:<\/strong> To guarantee a perfect cure every time, your <a href=\"https:\/\/plastisol-inks.com\/ja\/%e3%82%b9%e3%82%af%e3%83%aa%e3%83%bc%e3%83%b3%e5%8d%b0%e5%88%b7%e3%83%97%e3%83%a9%e3%82%b9%e3%83%81%e3%82%be%e3%83%ab%e3%82%a4%e3%83%b3%e3%82%af\/\">\u30d7\u30e9\u30b9\u30c1\u30be\u30eb\u30a4\u30f3\u30af<\/a> must reach a core temperature of 320\u00b0F(160\u2103) for at least 60 seconds. Doing this right ensures your prints survive 50+ industrial washes, stays elastic, and keeps your reputation solid.<\/p>\n\n\n\n<hr class=\"wp-block-separator has-alpha-channel-opacity\"\/>\n\n\n\n<h2 class=\"wp-block-heading\" id=\"why-we-wrote-this-the-solution-expert-perspective\">\u3053\u306e\u8a18\u4e8b\u3092\u66f8\u3044\u305f\u7406\u7531\uff1a\u30bd\u30ea\u30e5\u30fc\u30b7\u30e7\u30f3\u5c02\u9580\u5bb6\u306e\u8996\u70b9<\/h2>\n\n\n\n<p>We don&#8217;t just sell ink; we solve production nightmares. In the current 2026 market, where brands like Nike and Adidas demand strict oeko-tex 2026 compliance, &#8220;guessing&#8221; your dryer settings is a recipe for a lawsuit or a massive refund.<\/p>\n\n\n\n<p>Up to 65% of printing plant failures are caused by improper curing. We&#8217;ve spent years calibrating screen printing equipment to prevent this. This guide isn&#8217;t theoretical\u2014it&#8217;s what we use on our own factory floor.<\/p>\n\n\n\n<figure class=\"wp-block-image size-large\"><img fetchpriority=\"high\" decoding=\"async\" width=\"1024\" height=\"576\" src=\"https:\/\/plastisol-inks.com\/wp-content\/uploads\/2026\/04\/Plastisol-Ink-Not-Fully-Curing1-1024x576.jpg\" alt=\"\u30d7\u30e9\u30b9\u30c1\u30be\u30eb\u30a4\u30f3\u30af\u304c\u5b8c\u5168\u306b\u786c\u5316\u3057\u306a\u3044\u5834\u5408\u306f\uff1f\u5927\u91cf\u5370\u5237\u306e\u305f\u3081\u306e\u6e29\u5ea6\u30ac\u30a4\u30c9\" class=\"wp-image-8125\" title=\"\u30d7\u30e9\u30b9\u30c1\u30be\u30eb\u30a4\u30f3\u30ad\" srcset=\"https:\/\/plastisol-inks.com\/wp-content\/uploads\/2026\/04\/Plastisol-Ink-Not-Fully-Curing1-1024x576.jpg 1024w, https:\/\/plastisol-inks.com\/wp-content\/uploads\/2026\/04\/Plastisol-Ink-Not-Fully-Curing1-300x169.jpg 300w, https:\/\/plastisol-inks.com\/wp-content\/uploads\/2026\/04\/Plastisol-Ink-Not-Fully-Curing1-768x432.jpg 768w, https:\/\/plastisol-inks.com\/wp-content\/uploads\/2026\/04\/Plastisol-Ink-Not-Fully-Curing1-18x10.jpg 18w, https:\/\/plastisol-inks.com\/wp-content\/uploads\/2026\/04\/Plastisol-Ink-Not-Fully-Curing1.jpg 1200w\" sizes=\"(max-width: 1024px) 100vw, 1024px\" \/><figcaption>\u30d7\u30e9\u30b9\u30c1\u30be\u30eb\u30a4\u30f3\u30ad<\/figcaption><\/figure>\n\n\n\n<hr class=\"wp-block-separator has-alpha-channel-opacity\"\/>\n\n\n\n<h2 class=\"wp-block-heading\" id=\"the-2026-bulk-printing-cure-table\">2026\u5e74\u30d0\u30eb\u30af\u5370\u5237\u786c\u5316\u8868<\/h2>\n\n\n\n<figure class=\"wp-block-table\"><table class=\"has-fixed-layout\"><thead><tr><td><strong>\u30a4\u30f3\u30af\u306e\u7a2e\u985e<\/strong><\/td><td><strong>Core Temperature<\/strong><\/td><td><strong>Dwell Time<\/strong><\/td><td><strong>\u6700\u9069\u306a\u7528\u9014<\/strong><\/td><\/tr><\/thead><tbody><tr><td>Standard White Plastisol<\/td><td>320\u00b0F<\/td><td>60\u201390 sec<\/td><td>100% \u30b3\u30c3\u30c8\u30f3<\/td><\/tr><tr><td>Low-Cure Special Blends<\/td><td>280\u00b0F\u2013300\u00b0F<\/td><td>45\u201360 sec<\/td><td>Tri-blends &amp; Polyester<\/td><\/tr><tr><td><a href=\"https:\/\/plastisol-inks.com\/ja\/product\/%e3%82%b9%e3%82%af%e3%83%aa%e3%83%bc%e3%83%b3%e5%8d%b0%e5%88%b7%e7%94%a8%e3%83%91%e3%83%95%e3%82%a4%e3%83%b3%e3%82%af%e3%80%81%e7%b9%8a%e7%b6%ad%e7%94%a8%e9%ab%98%e5%af%86%e5%ba%a63d%e5%8a%b9%e6%9e%9c\/\">High-Density (3D) Ink<\/a><\/td><td>330\u00b0F<\/td><td>90\u2013120 sec<\/td><td>Canvas &amp; Workwear<\/td><\/tr><tr><td>Flash Curing (Between colors)<\/td><td>280\u00b0F<\/td><td>3\u20135 sec<\/td><td>Underbases<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<blockquote class=\"wp-block-quote is-layout-flow wp-block-quote-is-layout-flow\">\n<p><strong>\u73fe\u5834\u304b\u3089\u306e\u30d7\u30ed\u306e\u30d2\u30f3\u30c8\uff1a<\/strong> Don&#8217;t trust your dryer&#8217;s digital display blindly. We always recommend using thermolabels or a donut probe once a week to verify that the internal heat matches the readout. Surface temperature (what laser guns measure) is often 20\u00b0F higher than the core temperature.<\/p>\n<\/blockquote>\n\n\n\n<hr class=\"wp-block-separator has-alpha-channel-opacity\"\/>\n\n\n\n<h2 class=\"wp-block-heading\" id=\"how-to-get-started-calibrating-for-bulk\">\u59cb\u3081\u65b9\uff1a\u30d0\u30eb\u30af\u306e\u30ad\u30e3\u30ea\u30d6\u30ec\u30fc\u30b7\u30e7\u30f3<\/h2>\n\n\n\n<p>When we scale a client&#8217;s production to 5,000+ units, we start with a 3-point calibration test. This eliminates the variables like shop humidity or &#8220;cold spots&#8221; in the conveyor.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\" id=\"1-the-stretch-test-the-quick-check\">1. \u30b9\u30c8\u30ec\u30c3\u30c1\u30c6\u30b9\u30c8\uff08\u30af\u30a4\u30c3\u30af\u30c1\u30a7\u30c3\u30af\uff09<\/h3>\n\n\n\n<p>Once the garment is cool, grab the print and stretch it to about 1.5x its width. If it cracks, the molecules haven&#8217;t fused. If it snaps back like rubber, you\u2019re in the clear. Note: Overcuring (above 350\u00b0F) can actually cut ink elasticity by up to 40%, making the print brittle.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\" id=\"2-the-wash-test-the-gold-standard\">2\uff0e\u6d17\u6d44\u30c6\u30b9\u30c8\uff08\u30b4\u30fc\u30eb\u30c9\u30b9\u30bf\u30f3\u30c0\u30fc\u30c9\uff09<\/h3>\n\n\n\n<p>We tell our partners: &#8220;If it doesn&#8217;t survive the wash, it&#8217;s not finished.&#8221; Run a sample through a hot water cycle with industrial detergent. If you see dye migration or fading, your temperature wasn&#8217;t held long enough.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\" id=\"3-verification-of-2026-standards\">3\uff0e2026\u5e74\u898f\u683c\u306e\u691c\u8a3c<\/h3>\n\n\n\n<p>With the June 1st, 2026 oeko-tex updates, ensure your plastisol ink is free from regulated phthalates. Proper curing actually helps lock in these chemical compounds, making the garment safer for the end user.<\/p>\n\n\n\n<hr class=\"wp-block-separator has-alpha-channel-opacity\"\/>\n\n\n\n<h2 class=\"wp-block-heading\" id=\"best-practice-managing-the-heat-sink-effect\">Best Practice: Managing the &#8220;Heat Sink&#8221; Effect<\/h2>\n\n\n\n<p>In bulk printing, we often see shops &#8220;tiling&#8221; shirts (laying them too close on the belt). This is a mistake. Each shirt acts as a heat sink, absorbing the energy that should be going into the ink.<\/p>\n\n\n\n<p><strong>\u5f53\u793e\u306e\u30d9\u30b9\u30c8\u30d7\u30e9\u30af\u30c6\u30a3\u30b9\uff1a<\/strong> Keep a 3-inch gap between garments. This allows for even airflow and prevents &#8220;cold centers&#8221; where the ink stays raw. If you&#8217;re running heavy fleece, you must slow the belt speed down. Fleece holds moisture; that moisture has to evaporate before the ink can start to cure.<\/p>\n\n\n\n<hr class=\"wp-block-separator has-alpha-channel-opacity\"\/>\n\n\n\n<h2 class=\"wp-block-heading\" id=\"solving-the-cracking-mystery\">Solving the &#8220;Cracking&#8221; Mystery<\/h2>\n\n\n\n<p>If your ink is cracking after the first wash, it\u2019s almost always undercuring. Here is how we fix it:<\/p>\n\n\n\n<ul class=\"wp-block-list\">\n<li><strong>Check the Mesh:<\/strong> Are you using a mesh that&#8217;s too coarse? A thicker ink deposit takes longer to heat through.<\/li>\n\n\n\n<li><strong>Adjust the Height:<\/strong> If your heating elements are too high off the belt, you&#8217;re wasting energy. We keep ours at a consistent 3\u20134 inches.<\/li>\n\n\n\n<li><strong>Ink Additives:<\/strong> If you&#8217;re using textile additives to thin the ink, remember that some reducers can lower the flash point but may require a longer final cure.<\/li>\n<\/ul>\n\n\n\n<figure class=\"wp-block-image size-full\"><img decoding=\"async\" width=\"750\" height=\"750\" src=\"https:\/\/plastisol-inks.com\/wp-content\/uploads\/2026\/04\/Plastisol-Ink-Not-Fully-Curing.jpg\" alt=\"\u30d7\u30e9\u30b9\u30c1\u30be\u30eb\u30a4\u30f3\u30af\u304c\u5b8c\u5168\u306b\u786c\u5316\u3057\u306a\u3044\u5834\u5408\u306f\uff1f\u5927\u91cf\u5370\u5237\u306e\u305f\u3081\u306e\u6e29\u5ea6\u30ac\u30a4\u30c9\" class=\"wp-image-8126\" title=\"\u30d7\u30e9\u30b9\u30c1\u30be\u30eb\u30a4\u30f3\u30ad\" srcset=\"https:\/\/plastisol-inks.com\/wp-content\/uploads\/2026\/04\/Plastisol-Ink-Not-Fully-Curing.jpg 750w, https:\/\/plastisol-inks.com\/wp-content\/uploads\/2026\/04\/Plastisol-Ink-Not-Fully-Curing-300x300.jpg 300w, https:\/\/plastisol-inks.com\/wp-content\/uploads\/2026\/04\/Plastisol-Ink-Not-Fully-Curing-150x150.jpg 150w, https:\/\/plastisol-inks.com\/wp-content\/uploads\/2026\/04\/Plastisol-Ink-Not-Fully-Curing-12x12.jpg 12w, https:\/\/plastisol-inks.com\/wp-content\/uploads\/2026\/04\/Plastisol-Ink-Not-Fully-Curing-100x100.jpg 100w\" sizes=\"(max-width: 750px) 100vw, 750px\" \/><figcaption>\u30d7\u30e9\u30b9\u30c1\u30be\u30eb\u30a4\u30f3\u30ad<\/figcaption><\/figure>\n\n\n\n<hr class=\"wp-block-separator has-alpha-channel-opacity\"\/>\n\n\n\n<h2 class=\"wp-block-heading\" id=\"fa-qs-from-our-global-partners\">\u30b0\u30ed\u30fc\u30d0\u30eb\u30d1\u30fc\u30c8\u30ca\u30fc\u304b\u3089\u306e\u3088\u304f\u3042\u308b\u8cea\u554f<\/h2>\n\n\n<div id=\"rank-math-faq\" class=\"rank-math-block\">\n<div class=\"rank-math-list\">\n<div id=\"faq-question-1776925767849\" class=\"rank-math-list-item\">\n<h3 class=\"rank-math-question\">Q<strong>1. Can I cure plastisol with a simple heat gun for bulk orders?<\/strong><\/h3>\n<div class=\"rank-math-answer\">\n\n<p>Honestly? No. A heat gun is great for a DIY one-off, but for professional plastisol ink production, it&#8217;s impossible to maintain the 320\u00b0F consistency across a 12-inch design. You&#8217;ll end up with &#8220;islands&#8221; of cured ink surrounded by raw spots.<\/p>\n\n<\/div>\n<\/div>\n<div id=\"faq-question-1776925804543\" class=\"rank-math-list-item\">\n<h3 class=\"rank-math-question\">Q<strong>2. Why does my white ink peel while the black ink stays fine?<\/strong><\/h3>\n<div class=\"rank-math-answer\">\n\n<p>White ink is much denser\u2014it&#8217;s loaded with titanium dioxide. It reflects heat, while black ink absorbs it. We always suggest slowing the belt by 10% when switching from dark industrial inks to high-opacity white.<\/p>\n\n<\/div>\n<\/div>\n<div id=\"faq-question-1776925825005\" class=\"rank-math-list-item\">\n<h3 class=\"rank-math-question\">Q<strong>3. Is there a way to save energy during the curing process?<\/strong><\/h3>\n<div class=\"rank-math-answer\">\n\n<p>Yes. Modern &#8220;Low-Cure&#8221; inks, like the FN-INK series, can fuse at 280\u00b0F. This can save up to 25% in energy costs and prevents <a href=\"https:\/\/plastisolink.us\/it\/ultimate-guide-to-white-plastisol-ink-cure-techniques-for-screen-printing\/\" target=\"_blank\" rel=\"noreferrer noopener nofollow\">\u67d3\u6599\u79fb\u884c<\/a> on polyester. Check out our latest silicone leather trends for more low-heat material options.<\/p>\n\n<\/div>\n<\/div>\n<div id=\"faq-question-1776925869161\" class=\"rank-math-list-item\">\n<h3 class=\"rank-math-question\">Q<strong>4. What happens if I overcure the ink?<\/strong><\/h3>\n<div class=\"rank-math-answer\">\n\n<p>If you go above 350\u00b0F(177\u2103), you&#8217;re basically &#8220;burning&#8221; the plasticizers. The print will feel hard, look scorched, and will eventually crack because it has lost all its stretch.<\/p>\n\n<\/div>\n<\/div>\n<div id=\"faq-question-1776925932430\" class=\"rank-math-list-item\">\n<h3 class=\"rank-math-question\">Q<strong>5. How does humidity affect my dryer settings?<\/strong><\/h3>\n<div class=\"rank-math-answer\">\n\n<p>On rainy days, garments absorb moisture from the air. We&#8217;ve found that you need to increase your &#8220;dwell time&#8221; by about 15% on humid days to account for the energy used in evaporating that water.<\/p>\n\n<\/div>\n<\/div>\n<\/div>\n<\/div>\n\n\n<hr class=\"wp-block-separator has-alpha-channel-opacity\"\/>\n\n\n\n<h2 class=\"wp-block-heading\" id=\"final-thoughts-from-hong-rui-sheng\">\u30db\u30f3\u30fb\u30eb\u30a4\u30b7\u30a7\u30f3\u304b\u3089\u306e\u6700\u5f8c\u306e\u8a00\u8449<\/h2>\n\n\n\n<p>Curing isn&#8217;t just about heat; it&#8217;s about the marriage of Time + Temperature. As you expand into synthetic leather applications or new <a href=\"https:\/\/plastisol-inks.com\/ja\/scla%e3%82%b7%e3%83%aa%e3%83%bc%e3%82%ba\/\">pvc-free inks<\/a>, your calibration will be your best friend. Stay consistent, stay calibrated, and your bulk orders will stay perfect.<\/p>","protected":false},"excerpt":{"rendered":"<p>To guarantee a perfect cure every time, your plastisol ink must reach a core temperature of 320\u00b0F(160\u2103) for at least 60 seconds. Doing this right ensures your prints survive 50+ industrial washes, stays elastic, and keeps your reputation solid.<\/p>","protected":false},"author":11,"featured_media":8127,"comment_status":"closed","ping_status":"open","sticky":false,"template":"","format":"standard","meta":{"site-sidebar-layout":"default","site-content-layout":"","ast-site-content-layout":"default","site-content-style":"default","site-sidebar-style":"default","ast-global-header-display":"","ast-banner-title-visibility":"","ast-main-header-display":"","ast-hfb-above-header-display":"","ast-hfb-below-header-display":"","ast-hfb-mobile-header-display":"","site-post-title":"","ast-breadcrumbs-content":"","ast-featured-img":"","footer-sml-layout":"","theme-transparent-header-meta":"","adv-header-id-meta":"","stick-header-meta":"","header-above-stick-meta":"","header-main-stick-meta":"","header-below-stick-meta":"","astra-migrate-meta-layouts":"set","ast-page-background-enabled":"default","ast-page-background-meta":{"desktop":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-gradient":""},"tablet":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-gradient":""},"mobile":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-gradient":""}},"ast-content-background-meta":{"desktop":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-gradient":""},"tablet":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-gradient":""},"mobile":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-gradient":""}},"footnotes":""},"categories":[1],"tags":[150],"class_list":["post-8123","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-blog","tag-plastisol-ink"],"_links":{"self":[{"href":"https:\/\/plastisol-inks.com\/ja\/wp-json\/wp\/v2\/posts\/8123","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/plastisol-inks.com\/ja\/wp-json\/wp\/v2\/posts"}],"about":[{"href":"https:\/\/plastisol-inks.com\/ja\/wp-json\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"https:\/\/plastisol-inks.com\/ja\/wp-json\/wp\/v2\/users\/11"}],"replies":[{"embeddable":true,"href":"https:\/\/plastisol-inks.com\/ja\/wp-json\/wp\/v2\/comments?post=8123"}],"version-history":[{"count":5,"href":"https:\/\/plastisol-inks.com\/ja\/wp-json\/wp\/v2\/posts\/8123\/revisions"}],"predecessor-version":[{"id":8205,"href":"https:\/\/plastisol-inks.com\/ja\/wp-json\/wp\/v2\/posts\/8123\/revisions\/8205"}],"wp:featuredmedia":[{"embeddable":true,"href":"https:\/\/plastisol-inks.com\/ja\/wp-json\/wp\/v2\/media\/8127"}],"wp:attachment":[{"href":"https:\/\/plastisol-inks.com\/ja\/wp-json\/wp\/v2\/media?parent=8123"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"https:\/\/plastisol-inks.com\/ja\/wp-json\/wp\/v2\/categories?post=8123"},{"taxonomy":"post_tag","embeddable":true,"href":"https:\/\/plastisol-inks.com\/ja\/wp-json\/wp\/v2\/tags?post=8123"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}